logo
家
プロダクト
私達について
工場旅行
品質管理
私達に連絡しなさい
見積依頼
ニュース
TOGETHER HTL LTD
ホーム ニュース

Cooling Roller Temperature Uniformity: Which Design Holds the Face Even?

TOGETHER HTL LTD は非常に良い会社です。喜んで協力させていただきます。安全、効率的、プロフェッショナル、誠実、ハッピー!安定したサービスと製品を提供していただきありがとうございます。-----EUROPAT

—— 産業EUROPT

オンラインです
会社 ニュース
Cooling Roller Temperature Uniformity: Which Design Holds the Face Even?
最新の会社ニュース Cooling Roller Temperature Uniformity: Which Design Holds the Face Even?

Cooling Roller Temperature Uniformity: Which Design Holds the Face Even?

Quick Answer

For cross-face temperature uniformity, a counterflow double-spiral (duo-flow) double-shell cooling roller is the best general-purpose choice, holding ±1 °C across the working face and ±0.5 °C when spiral pitch is varied to offset coolant warming. Peripheral-drilled rolls achieve under 1 °C deviation but cost two to four times more. Open-cavity single-shell rolls typically show 4–10 °C edge-to-edge gradients on wide faces and should be limited to narrow, slow, low-load duties. Multi-zone temperature control improves any of these designs by 2–4 °C, but it compensates for edge losses rather than repairing a poor flow path.

Key Takeaways

· Cross-web temperature, not average roll temperature, determines gauge, haze and crystallinity

· The internal channel sets the convective coefficient; diameter and face length only set contact time

· Counterflow construction cancels the axial ramp that a single spiral accumulates

· Thermal crown turns a temperature error into a dimensional error of tens of microns

· Contact resistance at the web interface often dominates the heat path

· A uniformity guarantee must be tied to a flow, pressure drop and load condition

Summary Table

Item

Description

Function

Uniform extraction of heat from a cast or cooling web

Best design for uniformity

Counterflow double spiral with variable pitch

Typical face ΔT

±1 °C standard; ±0.5 °C matched; <1 °C peripheral drilled

Shell material

Forged alloy or stainless steel, hard chrome 80–120 µm

Surface finish

Ra 0.01–0.05 µm; mirror grades ≤ 0.01 µm

Applications

BOPP, BOPET, CPP, BOPA, cast film, optical, separator

Service life

10–15 years with treated water and scheduled descaling

 

Definition and Scope

A cooling roller is a rotating heat exchanger. Coolant enters through a rotary joint, travels a defined internal path, and leaves; the polymer web gives up heat through the shell wall into that coolant. "Temperature uniformity" is not a single property but the combination of four measurements taken at a defined load:

· Axial variation — maximum minus minimum surface temperature along the working face

· Circumferential variation — variation at a fixed point over one revolution

· Temporal drift — change at a fixed point over hours at steady load

· Shell-to-fluid difference — surface temperature minus coolant bulk temperature, which reveals whether the internal coefficient is adequate

A roller can be excellent on one of these and unusable on another. Suppliers and buyers frequently disagree because each is quoting a different number — which is the single most common reason a commissioning argument reaches the CASE STUDIES stage at all.

Working Principle

Heat transfer at the roll follows Q = h · A · ΔT. The area is fixed by roll size, the temperature difference is set by the process, and the design freedom sits almost entirely in h, the convective coefficient inside the channel.

In practical terms, four mechanisms decide the profile:

1. Flow regime. Reynolds number should stay above roughly 10,000. In laminar flow the same channel can lose more than half its effective coefficient, and the roll acquires a temperature map that no controller can flatten.

2. Coolant warming along the face. For a six-metre face removing 900 kW with 120 m³/h of water, the bulk rises about 6.5 °C between inlet and outlet. A single spiral passage experiences the entire gradient; a counterflow pair splits it into two opposed ramps that cancel.

3. Geometric equality. Every part of the face must see the same passage cross-section, the same clearance and the same velocity. One restricted passage creates a permanent warm band.

4. Hydraulic adequacy. A high-turbulence circuit may need more pump head than the existing chiller loop supplies. A starved channel performs worse than an open cavity, because it combines poor distribution with low velocity.


The Five Internal Architectures

Open-cavity single shell. Coolant enters one journal, crosses a largely open cylinder and exits the other, taking the path of least resistance through the centre. A slow boundary layer sits against the hot shell and insulates it, and low-velocity zones collect sediment that cannot be cleaned from outside. Face variation of 4–10 °C is normal on wide rolls.

Single spiral (mono-flow). A welded helical baffle creates a narrow continuous channel, forcing high-velocity flow against the shell. Heat transfer improves sharply, but the coolant warms as it travels, so the profile becomes a ramp — several degrees over four metres. Acceptable on medium widths where the set-point can be trimmed.

Counterflow double spiral (duo-flow). Two helical passages run side by side in opposite directions, so the supply-side gradient opposes the return-side gradient and the two cancel. With variable pitch — lead widened where coolant is coldest, tightened where warmest — a well-built roll holds ±1 °C, and ±0.5 °C on matched shells. This is the construction used in the BOPP CHILL ROLL and the wider PRS COOLING ROLL range.

Peripheral drilled (circumferential multi-hole). Deep bores are gun-drilled parallel to the axis a few millimetres beneath the working surface and fed from common headers. The conductive path collapses, response quickens, the shell stiffens, and deviation typically drops below 1 °C against roughly ±1.5 °C for deep-bore spiral designs. Cost rises steeply with face length, and header maldistribution becomes the dominant failure mode.

Multi-zone temperature control. Two to four independently fed zones along the face, each with its own supply and return through a multi-passage rotary union. Zoning compensates for edge losses where ambient cooling is highest, compressing 5–10 °C to ±1–2 °C on an average roll. It is a boundary-condition correction, not a heat-transfer improvement: inside each zone the local gradients remain.

Comparison Table

Design

Face ΔT at load

Relative cost

Best duty

Main limitation

Open-cavity single shell

4–10 °C

1.0×

Narrow, slow, low load

Short-circuiting, sedimentation

Single spiral mono-flow

2–4 °C

1.3–1.6×

Medium width

Axial ramp from coolant warming

Counterflow double spiral

±1 °C (±0.5 °C)

1.7–2.2×

Film casting, optical

Higher pressure drop

Peripheral drilled

<1 °C

2.5–4×

Optical, capacitor, separator

Header maldistribution, repair

Any design + multi-zone

−2 to −4 °C

+25–40%

Wide faces, retrofit

Masks rather than fixes

 

Benefits of a Uniform Face

The commercial case is not aesthetic. A flat thermal profile produces a flat gauge profile, which reduces the trimming that operators apply to the transverse orientation oven — trimming that moves the defect into optical properties instead of removing it. Uniform crystallinity across the width lowers break rates in the stretching oven. Reproducible contact gives reproducible haze and gloss on optical and metallised grades. Edge trim waste falls, because the edges stop running at a different temperature from the centre. And start-up after a shutdown becomes predictable rather than a process of chasing a profile for several hours. Downstream, the same profile carries into FILM CONVERTING ROLLS, where a CERAMIC COATING ROLL inherits whatever thermal history the caster created.

Applications and the Knowledge Graph

Previous process: extruder → filtration → die head → CASTING ROLL with pinning or air knife

Current process: cooling roller / chill roll / temperature control roll

Next process: MDO PREHEATING ROLL → MDO stretching → TDO → winding → corona → coating

In a sequential BOPP line the sheet leaves the die at 230–250 °C and must reach roughly 20–35 °C before the first preheat roll. Any width-wise unevenness in that quench is frozen in as a crystallinity and modulus gradient that no downstream oven can remove. The same physics governs BOPET, CPP, BOPA and cast film; the set-points differ, the mechanism does not. For the roll set surrounding this stage, see CASTING FILM ROLLS and BI-ORIENTED FILM ROLLS.

Material Comparison

Shell / coating

Thermal conductivity

Wear resistance

Corrosion resistance

Typical use

Carbon steel + hard chrome

High

High, 58–62 HRC

Medium

Standard film casting

Stainless steel + chrome

Medium

High

High

Humid or aggressive coolant

Chrome with matte texture

High

Medium

Medium

Release and gloss control

パブの時間 : 2026-11-16 17:19:21 >> ニュースのリスト
連絡先の詳細
TOGETHER HTL LTD

コンタクトパーソン: Mr. Maple

電話番号: +86 17778255675

ファックス: 86--311-80690567

私達に直接お問い合わせを送信 (0 / 3000)